welding · porosity · lack of fusion · heat tint · process
Common stainless weld defects: porosity, lack of fusion and heat tint
Porosity usually comes from poor shielding and contamination; lack of fusion relates to heat input and joint prep; heat tint signals insufficient shielding. Cleanliness and gas coverage are key.
Most stainless weld defects trace back to three things: cleaning, shielding and parameters.
1) Porosity: oil, moisture or rust on base metal or filler, insufficient shielding gas or excessive flow (turbulence entraining air), wind without shielding. Fix: thorough cleaning, check the gas path, add wind screens, bake filler per specification.
2) Lack of fusion / penetration: small bevel angle, large root face, low current, too fast travel, poor interpass cleaning. Fix: design the joint for the thickness, follow WPS/PQR, control interpass temperature and cleaning.
3) Heat tint: insufficient gas coverage or poor trailing shield. Tinted areas have reduced corrosion resistance and need pickling/passivation; critical parts should be welded without tint.
4) Distortion: use back-step and symmetrical welding with fixturing on thin sheet; straighten after welding if needed.
Acceptance: visual plus PT/RT/UT where required; for corrosion-critical parts, pickle and passivate after welding and run a blue-dot test. Weld quality comes from process discipline, not from rework.